Application and characterization of a novel PVDF

Scientific Reports volume 13, Article number: 3429 (2023) Cite this article

693 Accesses

Metrics details

The coatings on wood must sometimes give aesthetic and basic protection to wooden elements and prevent the development and transmission of microorganisms. Several polymers containing different nanoparticles have already been offered to day for this purpose. The research presents a novel poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP)/polyvinylpyrrolidone (PVP) polymer composite with MoO3 nanowires with the ability to form coating films on wood. The films of the developed coating exhibit elastic behaviour, which depends on the coating film thickness [tested wet film thicknesses (90, 180 and 360) µm]. The coating showed the ability to interact well with the surface of common beech (Fagus sylvatica L.) wood, in terms of wetting (contact angles of 15.6°), fast spilling on the surface, good penetration of the coating in wood structure and formation of up to 40 µm-thick films with excellent pull-off adhesion strength (6 MPa). An increased roughness of wood coated with C + MoO3 was a consequence of wood etching by the dimethylformamide solvent present in the coating. Moreover, the presence of C + MoO3 on wood made it considerably more hydrophobic, with contact angle of water raising to 123° from initially 46° measured on uncoated wood. The irradiation of wood surfaces with ultra-violet light resulted in visible colour changes on both uncoated and coated wood. The wood coated with C + MoO3 has a good resistance to water, alcohol and dry heat (grade 3 to 4). The antimicrobial testing showed that the presence of MoO3 in the coating plays an important role in the resistance of the coated wood to blue-stain fungi and mould development. The developed PVDF-HFP/PVP/MoO3 coating has an excellent ability to interact with the wood surface and has the potential to be used as a protection for wood in sensitive environments.

Microorganisms like bacteria, viruses and moulds are present all around us and have colonized all of the habitats in the world, including wood and wooden surfaces. If environmental conditions are suitable, these organisms can remain vital and transmittable for a considerable number of days if not months1. The fungal spores in living environment are spread around mostly from one person to another through the air flow and through contact with surfaces, like doors, tabletops, sittings, handles and similar. In general, the growth of moulds usually does not affect the mechanical properties of the wood, but if the wood remains moist long time enough, further development of fungi can cause the formation of soft rot, which can deteriorate the mechanical properties of the wood2. Moreover, as reported by Møller and co-workers3 and Viitanen and co-workers4, the presence of fungi and moulds like Aspergillus sp. (e.g. Aspergillus fumigatus), Aureobasidium pullullans, Alternaria alternata, Cladosporium sp. (e.g. Cladosporium herbarum, Cladosporium sphaerospermum), Mucor sp., Penicillium sp. (e.g. Penicillium brevicompactum), Stachybotrus sp. (e.g. Stachybotrus atra), and Fusarium solani, growing on wooden elements installed in living environment, can pose a serious threat for human health. Therefore, the antimicrobial protection of surfaces helps to prevent the spread of infection and diseases caused by microorganisms in the human population5.

The susceptibility of wood-based materials for infections with microbes can be determined by monitoring the growth of moulds and fungi on either uncoated or coated surfaces6. In general, each coating asset for surface treatment of wooden elements must meet several basic requirements. In order to successfully provide the expected functions of surface protection and a desired aesthetic appearance, the proper interactions between the wooden substrate and the coating are of crucial importance7. This way, good wetting of the wooden substrate, sufficient spilling and penetration of the coating in the wood structure defines the mechanical anchoring and adhesion of the coating film to the substrate. At the same time, the physical performance and resistance properties of the formed surface system are indicated by the surface hydrophobicity, resistance to cold liquids and changes in the surface appearance caused by the irradiation of ultra-violet (UV) light.

In the last decades, the trends in the development of new coating systems for wood are focused on searching and investigating the coating formulations with new binders and nanoparticles (e.g. TiO2, SiO2, ZnO, Al2O3, nanocellulose, graphene) as additives for improvement of various mechanical and physical properties8, as well as for preservation purposes9. Moreover, the need for effective and cost-affordable fungicidal agents (biocides) with long-acting and without risk to human health and the environment is extremely high.

Molybdenum trioxide (MoO3) was reported as one of the promising antimicrobial active substances10,11. In contrast to some other fungicidal compounds, the health risks in the case of MoO3 are minimal, as Mo is one of the essential elements in trace amounts and is a cofactor for the formation of enzymes in human bodies12. Otherwise, the 1 h-exposure of human keratinocyte cells (HaCaT) to MoO3 nanowires in concentration up to 1 mg × mL–1 after does not show any effect on cell survival13.

Minubaeva14 attributed the antimicrobial efficacy of MoO3 to its dissolution in water and the formation of antimicrobial molybdic acid (H2MoO4) (1):

Then, the H2MoO4 dissolves also into oxonium (H3O+) and molybdate (\({\text{MoO}}_{4}^{2 - }\)) ions, as follows (2):

while the protonation of the \({\text{MoO}}_{4}^{2 - }\) ions takes place simultaneously.

In principle, the diffusion of H3O+ ions through the cell wall of microbes causes an imbalance in pH value and the cell's enzyme and transport system. Therefore, for the antimicrobial action of MoO3 nanoparticles on the surface, the rate of MoO3 solubility in water (brought on the surface by microbes, air humidity, or cleaning) is of a critical in this process. Because that antimicrobial action is triggered by the presence of water in the liquid or vapour phase, this type of MoO3-containing nanocomposite can be an environmentally friendly sustainable solution because the use of detergents and disinfectants can be reduced.

The incorporation of MoO3 into polymeric binder allows the application of such polymer as a coating on various solid substrates, with controlled release rates and long-term use. Shafaei and co-authors15 reported the effect of different MoO3 crystal structures of micrometer size embedded in different polymer composites on antimicrobial activity against the bacteria S. aureus, E. coli and P. aeruginosa. The authors concluded that direct contact between the bacteria and MoO3 is needed that the H3O+ ions can diffuse through the bacterial membrane. All tests so far have been done with commercially available MoO3 with a micrometer size. Because the rate of solubility and consequent onset of antimicrobial activity depend on the specific surface area of MoO3, the nanoparticles (i.e. nanowires and nanotubes) of MoO3 have an advantage over the materials with MoO3 of micrometer size. In this manner, the high antimicrobial efficacy of MoO3 nanowires incorporated into poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP) and water-soluble polyvinylpyrrolidone (PVP) polymers was proven in our recent studies16,17.

Several examples of the use of coatings containing nanoparticles with antimicrobial properties well illustrate the potential use of such coating on furniture surfaces18,19. The aim of this research was to introduce the MoO3 nanoparticles into PVDF-HFP/PVP polymer composite acting as a binder to obtain a completely new type of coating for wood with improved physical properties and antimicrobial functionalities. Firstly, the basic properties (solids content and surface tension) of the synthetized liquid PVDF-HFP/PVP/MoO3 composite coating were determined. As the coating film thickness greatly influences the properties of the coating films and the properties of the surface systems, the coating was applied in three different wet-film thickness, namely 90 µm, 180 µm and 360 µm. The relation between the coating film thickness and its hardness was determined with a pendulum damping test. The wettability of wood with the coating was studied with contact angle (CA) measurements and by monitoring the spilling of the coating droplets over the surface after application on wood. After application of the coating on the surface of a wood, several properties of the coated wood were determined: Microstructure and surface roughness, hydrophobicity, stability against UV light irradiation, resistance properties, and the coating adhesion. Finally, the ability of the developed coating to prevent the growth of blue-stain fungi and moulds on the wood was tested.

Up to 3 μm-long MoO3 nanowires, with a diameter ranging from 100 to 150 nm, were obtained from Mo6S2I8 nanowires (Nanotul d.o.o., Ljubljana, Slovenia). These were synthesized in 236 h under chemical transport reaction in evacuated (104 Pa) quartz ampules and heated (800 °C) from molybdenum powder, sulfur powder and iodine beads (molar ratio 6:2:11.6). By oxidation at 285 °C for 24 h20 the MoO3 nanowires were grown in the orthorhombic crystal structure. Their solubility in pure water is (2.03 ± 0.09) mg × ml‒1 and the solutions reach the pH value of 3.8, as shown in a recent study17.

The polymer blend (C–MoO3) was synthesized by separately dissolving and mixing (120 min, 80 °C, 400 min–1) PVDF-HFP (Sigma-Aldrich, St. Louis, Missouri, USA) and PVP K30 (Sigma-Aldrich) in dimethylformamide (DMF, CARLO ERBA Reagents S.A.S., Milan, Italy). Then solutions of the polymers were mixed together and mixed for another 120 min. For the formation of nanocomposite, the MoO3 nanowires were dispersed in PVP solution and mixed for 120 min. Finally, the PVDF-HFP, PVP and MoO3 were mixed with a corresponding ratio 69:23:8 for another 120 min and the final coating product (C + MoO3) was obtained. As previously reported16, the C + MoO3 polymerizes and forms a solid film after drying for 120 min in a hot (80 °C) air atmosphere.

For the determination of solids content, a total of (1 ± 0.1) g of the liquid C + MoO3 was applied in three 50 mm diameter Petri dish and dried at a temperature of 125 °C for 60 min. The solids content (in %) was calculated from the initial C + MoO3 mass and its mass after drying, as prescribed by the standard EN ISO 325121.

The surface tension of the liquid C + MoO3 was determined according to Du Noüy ring method22 on processor tensiometer K100 (Krüss, Hamburg, Germany) using the corresponding software (Krüss LabDesk, Krüss). Five measurements were performed.

The coating films with wet thicknesses of 90 µm, 180 µm and 360 µm were created on the glass plates of 100 mm × 100 mm (3 plates per each film thickness) with a manual quadruple film applicator (Model 360, Erichsen GmbH & Co. KG, Hemer, Germany). The coating hardness was determined with pendulum-damped method23 using the König pendulum damping tester model 299/300 (Erichsen GmbH & Co. KG). The glass plates with applied coatings were placed for 120 min in an oven for drying (80 ± 2) °C and conditioned at (23 ± 2) °C and air relative humidity of (30 ± 5)% for 21 days afterwards. The coating hardness corresponded to the damping time of the pendulum swinging on the coating surface from 6° to 3° with respect to the normal axis (five measurements per sample). The longer the damping time, the harder the coating film.

The quartersawn common beech (Fagus sylvatica L.) sapwood planks, stored for two years in a room with air relative humidity of 30% and temperature 23 °C, were selected as a studied wooden substrate material. The gravimetrically determined nominal density of wood with (7.1 ± 0.4)% moisture content was (688.7 ± 24.5) kg × m–3. The wood was mechanically processed by sawing and peripheral planing into eight samples with dimensions (400 mm × 70 mm × 20 mm) and corresponding wood grain orientation longitudinal × radial × tangential (L × R × T). The samples were furtherly divided to the smaller samples for each analysis, as schematically presented in Fig. 1. All the analyses were conducted on the surfaces with R wood grain orientation, which were manually sanded with rotational-vibrational sanding machine (paper grit P180).

Distribution of wood samples preparation for different studies. The numbers present the sample size in individual wood grain direction (in millimeters): L—longitudinal, R—radial and T—tangential.

The wetting properties of wood surface with coating were estimated on the basis of the behavior of coating droplets after application on the surfaces of 3 uncoated samples (L = 50 mm). Five 5 µL-droplets of coating were applied on each sample with optical goniometer Theta (Biolin Scientific Oy, Espoo, Finland). The camera of goniometer enabled to record the motion of the droplet and to measure the CA of droplet following the Young–Laplace analysis24 continuously during first 60 s after application. The final CA was measured 2 h after droplet application.

After application on wood, the spilling of the coating droplets was determined by applying five 20 μL-droplets of coating from 20 mm above the sample surface using a pipette fixed on the stander. The spilling of the droplets 1, 2, 4, 6, 8, 10, 15, 20, 25, 30, 45, 60 and 7200 s after the application was recorded from above with a photo camera (D5600, Nikon, Tokyo, Japan). The photos were analyzed by measuring the spilling area (in mm2) of the droplets using the Fiji software (ImageJ 1.46d, Bethesda, Maryland, USA)25.

The surface systems on wood were formed by applying the coating with wet thicknesses of 90 µm, 180 µm and 360 µm with a manual quadruple film applicator (Erichsen GmbH & Co. KG) on two wood samples (L = 350 mm) for each film thickness. The coated wood samples were dried for 120 min in an oven at (80 ± 2) °C and afterwards conditioned at (23 ± 2) °C and air relative humidity of (30 ± 5)% for 7 days before further analyses.

The surface roughness of the uncoated and coated samples was examined on five selected spots on each sample with a LEXT OLS5000 confocal laser scanning microscope (CLSM, Olympus, Tokyo, Japan). The analyses at 5 × magnification provided the scanned area of (2560 × 2560) μm2. The microscope was equipped with a 405 nm laser light source with a maximum lateral resolution of 0.12 μm. The corresponding software (OLS50-S-AA, Olympus) was used to calculate the arithmetical mean height of the surfaces Sa26.

A droplet of C + MoO3 was deposited on an aluminum plate of (10 × 10 × 1) mm3 and polymerized. Moreover, two samples of about (5 × 5 × 5) mm3 were cut out of each coated wood sample. The microscopic structures of the cured C + MoO3 droplet, coated wood surfaces and their cross-sections were analyzed with a scanning electron microscope Quanta 250 (Thermo Fisher Scientific, Hillsboro, USA). A gold conductive layer was sputtered on the samples prior to observations. The images were acquired with the Everhart–Thornley detector in high vacuum (0.078 Pa) with an electron source voltage of 5.0 kV, at a working distance of 10 mm, a spot size of 3.0 nm, and by the time of electron beam passage through the sample of 45 μs.

In order to detect the hydrophobic characteristics of wood coated with coating films of different thicknesses, again the optical goniometer Theta (Biolin Scientific Oy) was used. Ten 5 µL-droplets of demineralized water were applied on the samples (L = 30 mm) coated with each film thickness and the formed CAs were monitored continuously for 60 s.

The coated wood samples were exposed to UV light originating from 450 mm-distant Ultra-Vitalux 300 W bulb (Osram, Munich, Germany) for 96 h. The colour changes of the samples during exposure to UV light were monitored after 3, 6, 24, 48, 72, and 96 h by measuring L* (0 = black, 100 = white), a* (negative = green, positive = red) and b* (negative = blue, positive = yellow) colour space components using the spectrophotometer SP62 (X-Rite, Grand Rapids, USA) with the D65 light type. Colour changes of the sample surfaces after the certain time of exposure to UV (ΔE*) were calculated according to Eq. (3):

where n present the parameter value after a certain interval of exposure to UV and 0 present the initial value of a certain parameter. Meanwhile, the photodegradation of the uncoated and coated samples due to UV light irradiation was quantified with attenuated total reflection Fourier transform infra-red (ATR-FTIR) spectrometer Spectrum Two (PerkinElmer Inc., Waltham, USA). The spectra were measured in 3 spots (16 scans per spot) on individual sample, in a wavelength region from 600 to 4000 cm–1 at a resolution of 0.5 cm–1. The relevant absorption bands were interpreted with the Spectrum software (version 10.5.3, PerkinElmer Inc.).

The resistance of the surface to cold liquids was determined according to the method prescribed by EN 1272027. Soft filter paper disks (diameter 25 mm, grammage 450 g × m–2) were immersed for 30 s in deionized water and water solution (48%) of ethanol28. Three disks soaked into each liquid were placed on the surface of the coated samples, immediately covered with a Petri dish and left as so for 1 h. After the exposure period, the disks were removed, and the remainder of the liquids was carefully wiped off with a soft paper towel.

In order to determine the resistance of the surface systems to dry heat29 the aluminum disks were heated to 85 °C and 200 °C and placed on the surfaces of the coated samples for 20 min and removed afterwards.

After 24 h, all the tested surfaces were cleaned, examined for damage in a standardized viewing cabinet and rated according to a numerical evaluation code from 5 to 1 (5—no change, 1—severe change).

For determination of coating adhesion ten aluminum dollies were bonded to each coated surface using an epoxy adhesive (Endfest 300, UHU, Bühl, Germany). After 24 h, the cured epoxy adhesive around the perimeter of each dolly was cut to the substrate and the dollies were pulled-off at a tensile stress rate of 1 MPa × s–1 using a PosiTest AT pull-off adhesion tester (DeFelsco Corporation, Ogdensburg, USA)30. Besides the breaking strength, the fractures between the dollies and the surface of coated wood were visually assessed.

The blue-stain fungal test was performed according to modified standard EN 152-131, by exposing the samples coated with C + MoO3, C–MoO3 and uncoated samples (10 samples of each series) to blue-stain fungi Aureobasidium pullulans (de Barry) Arnaud (ZIM L060) and Sclerophoma pithyophila (Corda) Hohn (ZIM L070) for the period of 8 weeks. The specimens were submerged to spore suspension and afterwards transferred to experimental jars (250 mL) with 15 mL of spore suspension. After the termination of the exposure period, the evaluation of surface blue-staining on each specimen was visually rated on a scale of 0–3 with the naked eye and light microscope, using the criteria prescribed in standard31 (Table 1).

The resistance of samples to mould overgrowth was assessed according to a modified American wood protection association standard E24-1232. The test took place in a moulds box with a controlled temperature of 25 °C and relative air humidity of (95–98)% for 8 weeks. Five samples of (60 × 20 × 5) mm (L × R × T) from each series were placed on a mesh rack above the water with moist soil with treated surfaces facing the upside. The soil was inoculated with a suspension of spores and mycelium of Aureobasidium pullulans (d. By.) Arnaud, Aspergillus niger Van Tiegh, Alternaria tenuissima (Kunze) Wiltshire, and Penicillium citrinum Thom. Mould coverage of the samples was monitored by scanning the samples weekly. Mould growth on each specimen was visually rated on a scale of 0–4 with the naked eye and light microscope, using the criteria proposed by Johansson and co-workers33.

The non-volatile content in the C + MoO3 was (21 ± 2)%. The surface tension of the liquid C + MoO3 with a temperature of 23 °C was (33.22 ± 0.04) mN × m–1, while heating the liquid C + MoO3 to 80 °C decreased its surface tension to (29.87 ± 0.07) mN × m–1.

In the pendulum test for measuring of hardness of a coating, amplitude of oscillation is measured as a function of time. In general, the hardness of a coating is greatly related to its thickness; the harder is the analyzed coating film, the greater is the oscillation time of the pendulum34. Damping of the oscillations is also affected by elastic deformations present in a coating film. The damping time on the uncoated glass was (175 ± 1) s. Among the C + MoO3 films, the longest damping time (126 ± 5) s, i.e. the smallest damping effect, was measured on the 90 µm-thick film (Fig. 2). With the increase of the film thickness to 180 µm, the damping time shortened for 21% to (99 ± 3) s. However, on the thickest C + MoO3 film (360 µm) the damping time shortened only slightly (3.5%) to (96 ± 3) s. The results show that the C + MoO3 films exhibit elastic behavior, because their hardness is not linearly correlated with the coating film thickness. The damping times were comparable to the damping times measured on films of indoor wood coatings35, but notably shorter than on films of exterior wood coatings36.

Damping times determined with pendulum hardness tester on a glass with applied C + MoO3 films with different wet film thicknesses and on uncoated glass.

The evolution of CAs of C + MoO3 droplets and spilling areas after application of the coatings on beech wood substrate are shown in Fig. 3. The C + MoO3 expressed good wetting abilities on the surface of the wood. In average, the initial detected CA was (26.4 ± 3.2)°. With time, it gradually decreased to (11.5 ± 3.2)° in 60 s of measurements. After 120 min, the CA of the droplets decreased to (7.1 ± 3.2)° and completely wetted the surface of wood.

Evolution of the spilling area and contact angle of C + MoO3 droplets applied on beech wood. The photos are showing the top-view photos of the applied droplets after correspondent time after deposition. The length of the scale bar is 5 mm.

The spilling area of the C + MoO3 1 s after droplet deposition on the surface of wood was (15.6 ± 5.3) mm2 and rapidly increased to (28.3 ± 5.0) mm2 in the first 5 s after deposition. After 60 s and 120 min of observations, the spillings of C + MoO3 were (46.7 ± 7.3) mm2 and (53.8 ± 9.3) mm2, respectively.

The images and measured arithmetic mean surface roughness of uncoated (sanded) wood and wood coated with different thicknesses of wet films of C + MoO3 are shown in the Fig. 4. The coated surfaces of wood were rougher than uncoated surfaces of wood. Moreover, the roughness of coated wood surface increased with the larger thickness of C + MoO3 film. The application of the thinnest (90 µm) C + MoO3 film increased the roughness of samples from (7.7 ± 0.8) µm to (10.6 ± 0.6) µm, or for about 38%. The application of thicker (180 µm) C + MoO3 film increased the roughness of wood even more (to (16.0 ± 0.4) µm), that is about 110% increase. As reported in different studies, the dimethylformamide, which was used in our coating, as an ionic liquid, can dissolve cellulose37, hemicelluloses38 and lignin39 in wood. Therefore, the increasing surface roughness with increasing coating film thickness is most probably related with the greater content of dimethylformamide solvent in the C + MoO3 film, which caused the etching of the underlying wood surface. However, the application of the thickest (360 µm) coating film did not increase the surface roughness substantially any further ((16.2 ± 0.5) µm). In this case, despite the etching of wood surface by the dimethylformamide solvent, the content of the remaining polymer blend on the wood surface seemed to be thick enough to hinder the etching effect.

Chart shows the arithmetic mean surface roughness of uncoated wood and wood coated with different thicknesses of C + MoO3 wet films. The images on the right show the appearance of the samples surface: left column show the photos of the surfaces (length of the scale bar is 10 mm), right column show the 3D images of each type of analyzed surface as obtained with CLSM (analyzed surface of (2560 × 2560) μm2).

Images in Fig. 5a show the microstructure of the cured C + MoO3 droplet. A more detailed analysis of the coated wood samples with SEM revealed the microstructure of the samples' surface and the microstructure of the samples' cross-sections with the properties of the interface between wood and C + MoO3 film (Fig. 5b‒d). The analysis revealed the presence of MoO3 nanowire clusters embedded in the polymer over the entire surface of the coated samples. The surface porosity of the wood beech substrate is reflected in the uneven and porous film of C + MoO3. The thicker the coating film was, the smaller pores with a diameter of up to few tens of µm were on the surface. On the sample coated with the thickest (360 µm) C + MoO3 film, clusters of MoO3 nanowires were no longer detected.

SEM images in (a) show the microstructure of the cured C + MoO3 droplet (left) and the MoO3 nanowires embedded in the PVDF-HFP/PVP polymer (right). Images (b)–(d) show the surface of wood coated with different wet film thicknesses of C + MoO3: (b) 90 µm, (c) 180 µm and (d) 360 µm. The left images show the surfaces structure: Triangular arrows are pointing the pores in the coating films, while the clusters of MoO3 nanowires are encircled with the dashed lines. The right images show the cross-sections structure: The clear transition between cellular wooden substrate (bottom) and the film of C + MoO3 is clearly visible only in (c) and (d). The estimated dry film thicknesses present the distance between the contradictory arrows.

The thicknesses of the dry coating films were estimated on the cross-section images of the coated samples. The dry C + MoO3 film thickness on sample coated with wet film thickness of 90 µm varied from about (3 to 8) µm, on sample coated with 180 µm-thick film from about (10 to 16) µm and on sample coated with 360 µm-thick film from about (15 to 40) µm.

The behavior of water droplets deposited on coated wood was a good indicator of the ability of the C + MoO3 film of particular thickness to protect the wooden substrate from water. The uncoated wood surface showed a notably higher affinity to absorb water droplets than the wood surface coated with C + MoO3 films (Fig. 6). After deposition on uncoated wood, the water droplets formed the CA with the wood surface of (45.7 ± 8.5)°. In 60 s of monitoring, the CA decreased to (31.7 ± 8.4)° due to the penetration of water into the substrate and spreading over the wood surface. The wood surface coated with C + MoO3 exhibited hydrophobic properties, which depended on the C + MoO3 film thickness. The developed CAs of water decreased only by about 1° during the 60 s measurements, regardless of C + MoO3 film thickness. The wood surface coated with the thinnest film of C + MoO3 exhibited the most hydrophobic character with initial water CA of (122.8 ± 7.4)°. The initial CAs of water droplets on surfaces of wood coated with 180 µm and 360 µm of C + MoO3 were lower (111.6 ± 9.3 and 98.2 ± 2.9)°, respectively. These surfaces can still be denoted as hydrophobic40. This brings to the conclusion that the thinner is C + MoO3 film, the higher is the hydrophobic character of the coated wood surface. The reason for this lays in the influence of C + MoO3 film thickness on the surface roughness. The larger amount of C + MoO3 on wood leads to increased surface roughness (etching of wood) and to lower developed CAs of water droplets. The relation between the higher surface roughness of poly-dimethylsiloxane and lower water CAs was, as for example, reported by Juárez-Moreno and co-authors41.

Evolution of water droplets CAs after deposition on the uncoated beech wood surface and on surfaces coated with C + MoO3 films different thickness. The images on the right show the photos of the water droplets acquired 2 s after deposition on each type of surface. The length of the scale bar is 1 mm.

The irradiation of the coated wood samples with UV light caused the changes in the colour of the samples shown in the Fig. 7. On all samples, the most intensive changes in colour occurred during the first 6 h of exposure, and then to the final 96 h, the change rates gradually slowed down. The uncoated wood samples became darker (ΔL* = – 8.7), more reddish (Δa* = 5.0) and yellower (Δb* = 3.8), signalizing the structural changes in lignin42. Since the C + MoO3 films were semi-transparent, the observed colour changes on the coated samples resulted from combined changes that took place in the wood surface and coating films. After 96 h of exposure to UV light, the largest changes (ΔE* = 14.4) were observed in samples coated with 90 µm-thick coating film, followed by the samples coated with 180 µm-thick coating film (ΔE* = 13.3) and uncoated wood (ΔE* = 10.8). The colour changes of samples coated with 360 µm-thick coating film were lower (ΔE* = 4.8), but still intensive enough to be detected with the naked eye (ΔE* ≥ 2)43.

Colour changes of uncoated and coated wood samples during 96 h of irradiation with UV light. The length of the scale bar is 10 mm.

The spectra obtained with ATR-FTIR spectrometer on the uncoated wood surface and wood surface coated with C + MoO3 of different film thicknesses before and after exposure to UV light are shown in Fig. 8.

ATR-FTIR spectra of wood and coated samples in the wavelength region between (800 and 1800) cm‒1 and region between (2700 and 3700) cm‒1, recorded before (unexposed) and after 96 h of exposure to UV light.

The C + MoO3 films hindered the chemical composition of uncoated wood, regardless of film thickness. By increasing the C + MoO3 film thickness, the broad peak of hydroxyl (OH) groups between (3500 and 3200) cm–1 decreased. The peaks at 2930 cm–1 (signalizing asymmetric CH2 stretching) and 2840 cm–1 (signalizing symmetric CH2 stretching) intensified with increased C + MoO3 film thickness. These peaks originate from crystalline cellulose in wood44 and identify the dissolution of wood tissue by C + MoO3. The peak at 1740 cm–1 typical for C=O stretch in hemicelluloses (xylan)45, completely disappeared, which is another indicator of wood dissolvement by C + MoO3. On the other hand, a new main peak between (1660 and 1680) cm–1, with a shoulder peak at 1700 cm–1 (attributed to C=O stretching of PVP) appeared46. The shift of the main peak from 1660 cm–1 to 1670 cm–1and 1680 cm–1 with higher C + MoO3 thickness (from 90 to 180 and 360) µm is related to the intermolecular interaction between the polymers47,48. The peak at 1670 cm‒1 was present due to C=O bound by PVP–PVP dipole interactions or having weak hydrogen bonding to another species. In the case of C=O groups strongly bound to another species, the peak was more shifted to 1660 cm‒1.

Similarly, another peak at 1400 cm–1 signalizing CH2 wagging of PVDF-HFP and PVP in polymer blend49 raised with larger thickness of C + MoO3 on wood. The peak at 1280 cm–1 on coated wood is assigned to β phase of PVDF50 and was slightly intensified with larger thickness of C + MoO3. An indicative peak on wood coated with C + MoO3 at 1190 cm–1 is assigned to antisymmetric stretching of CF251 and intensifies with amount of C + MoO3. The peak at 1050 cm–1 as the most intensive on wood indicating the C–O deformation in cellulose, symmetric C–O–C stretching of dialkyl ethers, and aromatic C–H deformations in lignin52 completely disappeared with application of C + MoO3 on wood. Instead, the peak at 990 cm–1, corresponding to the α-phase of PVDF–HFP51 appeared. Another two peaks at 870 cm–1 (indicating γ phase of PVDF-HFP) and 840 cm–1 (indicating β phase of PVDF, –CH2– rocking and –CF2– stretching) were observed53. All these three peaks were promoted with greater film thickness of C + MoO3 on wood.

The exposure of uncoated wood to UV light caused a slight increase of the peak at 2930 cm–1 (C–H asymmetrical and symmetrical stretching54) and a more notable rise of peaks at 1680 cm–1 and 1600 cm–1, indicating oxidation of lignin55 and presence of C–C unsaturated linkages in aromatic rings of lignin56. An intensified shoulder peak at 1080 cm–1 was attributed to the rearrangements in lignin, specifically the aromatic C–H in plane deformation in guaiacyl units and C–O deformation in primary alcohol57. On wood coated with C + MoO3, the peaks at 2930 cm–1 and 2850 cm–1 diminished with the exposure of coated surfaces to UV light. This indicates the degradation of the remaining cellulose in coated wood by UV light44. Moreover, after the exposure to UV light caused the formation of succinimide ((CH2)2(CO)2NH) groups and consequently the main peak at 1680 cm–1 remained without a shoulder peak at 1700 cm–1. The UV irradiation triggered additional crosslinking reaction and photodegradation of PVP in C + MoO346,58.

The results of resistance properties of coated wood surfaces to various impacts are presented in Table 2. The left half of the images shows the assessed surfaces before the resistance property tests, and the right half of the images the appearance of the test surfaces after the completed test. The resistance of the coated wood surfaces to water was rated as good (grade 3), and the damage caused was the same by all three thicknesses of the coating film. The exposure to water probably caused a partial dissolution of the coating since the underlying wood became more visible after the exposure. A similar level of damage was observed by determining the resistance of the surfaces to alcohol (grade 3), while the surface coated with 360 µm was more resistant to alcohol (grade 4). The exposure of the surfaces to the dry heat caused a minor change in colour of the surfaces, and the grade was in all cases 4.

When compared with the common wood coatings reaching the pull-off adhesion strengths between 2 and 3 MPa59, the adhesion of the developed C + MoO3 coating to wood can be referred as very high, since the values exceeded 6 MPa. Moreover, the adhesion of the coating to the wood substrate was not influenced by the coating film thickness and was generally the same by all of the thicknesses studied (Fig. 9). As seen in the images above the chart in Fig. 9, the adhesion failure between the detached dolly and the coated surface was representative (approximately 60%), while the failure was partially cohesive in the wooden substrate. This indicated that the adhesion of the coating to wood exceeded the cohesive strength of wood and adhesion between the dolly and coated surface.

Pull-off adhesion strength of coating films with different wet film thicknesses. The images above the chart show the representative types of failures. The length of the scale bars is 10 mm.

The results of the blue-staining fungal test are presented in the Table 3. The images show the surfaces of exemplary samples from each series before the test start, and surfaces and cross-sections of the same samples after the test was completed in 8 weeks. The given grades of the samples overgrown with blue-stain fungi correspond to the visual assessment with the naked eye and microscopical investigations. The results of the blue-stain fungal test showed that uncoated samples and samples coated with C–MoO3 were more overgrown with blue-stain fungi and rated as 3 (average attack). The presence of blue-stain fungi hyphae was observed through the entire cross-section of the samples on both types of samples. The assessment of the samples coated with C + MoO3 was more challenging, as the blue colour of the fungal hyphae was slightly hardly distinguishable from the blue surface of the coated wood. However, the blue-staining on C + MoO3 samples predominantly appeared on the side surfaces and the edges of the coated surface, while the center of the coated surface remained intact. For these reasons the C + MoO3 samples were rated as 2 (slight attack).

The results of the resistance to mould growth are presented in Table 4. The images show the surfaces of exemplary samples from each series before the start of the test and the images of the same surfaces during 8 weeks of exposure to mould growth in humid environment. As detected with the naked eye, the mould appeared on all three types of samples after completed 7 weeks of exposure. Due to the darker colour of C + MoO3, the light-shaded mould was especially visible on samples coated with C + MoO3. However, darker conidiophores were detected only on the uncoated samples and samples coated with C–MoO3, but not on samples coated with C + MoO3. At the end of exposure, the presence of well-developed conidiophores was confirmed with the microscope on the uncoated sample, giving these the grade 4. On the samples coated with C–MoO3, the conidiophores seemed to be at the beginning of development (grade 3). On the samples coated with C + MoO3 no development of conidiophores was detected after the completed test, and the grade 0 was given to this set of samples.

To get a better overview of the properties of C + MoO3, these are compared in Table 5 with the properties of the commercially available interior coatings whose properties were reported in the listed references. It should be mentioned that many of these parameters are defined by the properties of the coating itself (e.g. type of binder), the properties of the coating system (e.g. number of layers) or the properties of the surface system, which includes also the properties of the substrate (e.g. type of wood). The properties of C + MoO3 were in some respects more and in some respects less comparable to the values from the other studies. For example, the hardness of C + MoO3 was even up to 2-times higher than usually due to the thinner layers. The same is true for the roughness of the coated wood surface; a greater dry film thickness of the coating smooths the surface of the wood substrate more effectively. The colour changes caused by artificial weathering additionally depend on the weathering parameters (temperature and humidity conditions, type of light source, exposure time, etc.), so it is difficult to compare the ΔE* values with those obtained in other studies. Once again, good performance was confirmed in terms of C + MoO3 adhesion and mould resistance of wood coated with C + MoO3.

A novel PVDF-HFP/PVP polymer composite containing MoO3 nanoparticles with the ability to form coating films was successfully synthesized. At first, the experiments presented in the article showed that the hardness of the C + MoO3 films depended on the coating film thickness (tested wet film thicknesses 90 µm, 180 µm and 360 µm). The developed coating showed the ability to form the surface system with the surface of beech wood. C + MoO3 expressed good wetting abilities on the wood surface, reaching the initial values of CAs of about 15.6° together with fast spilling on the wood surface. The roughness of coated wood surface increased with the larger thickness of C + MoO3 film, due to the etching of the wood surface by the dimethylformamide solvent in the coating. The C + MoO3 well penetrated in the wood surface microstructure, forming the cured coating films with thickness from only 3 µm (applied 90 µm) to 40 µm (applied 360 µm). The presence of C + MoO3 on a wood surface made it considerably more hydrophobic when compared to uncoated wood, reaching the values of water CAs up to about 123°. The irradiation of wood surface coated with C + MoO3 with UV light caused visible colour changes on the tested samples, which was together with oxidation of lignin and degradation of cellulose in wood, a consequence of the photodegradation of PVP in C + MoO3 coating. The coated wood surfaces exhibited good resistance to water, alcohol and dry heat (grade 3–4), while the adhesion of the C + MoO3 to the wood surface was excellent (6 MPa), regardless of the coating film thickness. The antimicrobial testing showed that the presence of MoO3 in the developed coating played an important role by the resistance to blue-stain fungi and mould development. While the uncoated wood samples and samples coated with C–MoO3 experienced an average attack (grade 3), the samples coated with C + MoO3 experienced a slight attack (grade 2) from the blue-stain fungi. The contribution of MoO3 presence was even more evident by testing the resistance of the samples to mould growth. After 7 weeks of testing, the conidiophores were well developed on the uncoated samples (grade 4), slightly less on samples coated with C–MoO3 (grade 3), but absent on the samples coated with C + MoO3 (grade 0).

In conclusion, the developed PVDF-HFP/PVP polymer composite with MoO3 nanoparticles has a good ability to interact with wood surfaces and can potentially be used as a protective coating for wood, in terms of protection to physical impacts as well as to protect the wood from microbes.

The datasets used and/or analysed during the current study available from the corresponding author on reasonable request.

Van Doremalen, N. et al. Aerosol and surface stability of SARS-CoV-2 as compared with SARS-CoV-1. N. Engl. J. Med. 382(16), 1564–1567. https://doi.org/10.1056/NEJMc2004973 (2020).

Article PubMed Google Scholar

Uzunovic, A., Byrne, T., Gignac, M. & Dian-Qing, Y. Wood discolourations wood discolourations & their prevention with an emphasis on bluestain. Special Publication SP-50, ISSN 1917–4328, FPInnovations (2008).

Møller, E. B., Andersen, B., Rode, C. & Peuhkuri, R. Conditions for mould growth on typical interior surfaces. Energy Procedia 132, 171–176. https://doi.org/10.1016/j.egypro.2017.09.680 (2017).

Article Google Scholar

Viitanen, H. et al. Towards modelling of decay risk of wooden materials. Eur. J. Wood Prod. 68, 303–313. https://doi.org/10.1007/s00107-010-0450-x (2010).

Article Google Scholar

Elashnikov, R. et al. Physically switchable antimicrobial surfaces and coatings: General concept and recent achievements. Nanomaterials 11, 3083. https://doi.org/10.3390/nano11113083 (2021).

Article CAS PubMed PubMed Central Google Scholar

Gobakken, L. R. & Vestøl, G. I. Surface mould and blue stain fungi on coated Norway spruce cladding. Int. Biodeterior. Biodegrad. 75, 181–186. https://doi.org/10.1016/j.ibiod.2012.10.001 (2012).

Article CAS Google Scholar

Miklečić, J., Lončarić, A., Veseličić, N. & Jirouš-Rajković, V. Influence of wood surface preparation on roughness, wettability and coating adhesion of unmodified and thermally modified wood. Drv. Ind. 73(3), 261–269. https://doi.org/10.5552/drvind.2022.0016 (2022).

Article Google Scholar

Kaboorani, A., Auclair, N., Riedl, B. & Landry, V. Mechanical properties of UV-cured cellulose nanocrystal (CNC) nanocomposite coating for wood furniture. Prog. Org. Coat. 104, 91–96. https://doi.org/10.1016/j.porgcoat.2016.11.031 (2017).

Article CAS Google Scholar

Tomak, E. D., Yazici, O. A., Sam Parmak, E. D. & Gonultas, O. Influence of tannin containing coatings on weathering resistance of wood: Combination with zinc and cerium oxide nanoparticles. Polym. Deg. Stab. 152, 289–296. https://doi.org/10.1016/j.polymdegradstab.2018.03.012 (2018).

Article CAS Google Scholar

Zollfrank, C., Gutbrod, K., Wechsler, P. & Guggenbichler, J. P. Antimicrobial activity of transition metal acid MoO3 prevents microbial growth on material surfaces. Mater. Sci. Eng. C 32(1), 47–54. https://doi.org/10.1016/j.msec.2011.09.010 (2012).

Article CAS Google Scholar

Krishnamoorthy, K., Veerapandian, M., Yun, K. & Kim, S. J. New function of molybdenum trioxide nanoplates: Toxicity towards pathogenic bacteria through membrane stress. Colloids Surf. B Biointerfaces 112, 521–524. https://doi.org/10.1016/j.colsurfb.2013.08.026 (2013).

Article CAS PubMed Google Scholar

Yoshida, M. et al. Molybdenum balance in healthy young Japanese women. J. Trace Elem. Med. Biol. 20(4), 245–252. https://doi.org/10.1016/j.jtemb.2006.07.004 (2006).

Article CAS PubMed Google Scholar

Božinović, K. et al. In-vitro toxicity of molybdenum trioxide nanoparticles on human keratinocytes. Toxicology 444, 152564. https://doi.org/10.1016/j.tox.2020.152564 (2020).

Article CAS PubMed Google Scholar

Minubaeva, Z. UV Spectroscopic Studies of the Hydrothermal Geochemistry of Molybdenum and Tungsten. Doctoral dissertation, ETH Zurich, ETH (2007).

Shafaei, S., Dörrstein, J., Guggenbichler, J. P. & Zollfrank, C. Cellulose acetate-based composites with antimicrobial properties from embedded molybdenum trioxide particles. Lett. Appl. Microbiol. 64(1), 43–50. https://doi.org/10.1111/lam.12670 (2016).

Article CAS PubMed Google Scholar

Gradišar Centa, U., Kocbek, P., Belcarz, A., Škapin, S. D. & Remškar, M. Polymer blend containing MoO3 nanowires with antibacterial activity against staphylococcus epidermidis ATCC 12228. J. Nanomater. https://doi.org/10.1155/2020/9754024 (2020).

Article Google Scholar

Gradišar Centa, U. et al. Novel nanostructured and antimicrobial PVDF-HFP/PVP/MoO3 composite. Surf. Innov. 9(5), 256–266. https://doi.org/10.1680/jsuin.20.00073 (2021).

Article Google Scholar

Wei, X., Yang, Z., Leng Taya, S. & Gao, W. Photocatalytic TiO2 nanoparticles enhanced polymer antimicrobial coating. Appl. Surf. Sci. 290, 274–279. https://doi.org/10.1016/j.apsusc.2013.11.067 (2014).

Article ADS CAS Google Scholar

Gerullis, S. et al. Thin antimicrobial silver, copper or zinc containing SiOx films on wood polymer composites (WPC) applied by atmospheric pressure plasma chemical vapour deposition (APCVD) and sol–gel technology. Eur. J. Wood Prod. 76, 229–241. https://doi.org/10.1007/s00107-017-1220-9 (2018).

Article CAS Google Scholar

Varlec, A., Arčon, D., Škapin, S. D. & Remškar, M. Oxygen deficiency in MoO3 polycrystalline nanowires and nanotubes. Mater. Chem. Phys. 170, 154–161. https://doi.org/10.1016/j.matchemphys.2015.12.033 (2016).

Article CAS Google Scholar

EN ISO 3251. Paints, Varnishes and Plastics: Determination of Non-volatile-Matter Content (ISO 3251:2019) (European Committee for Standardization, 2019).

Du Noüy, P. L. An interfacial tensiometer for universal use. J. Gen. Physiol. 7, 625–631. https://doi.org/10.1085/jgp.7.5.625 (1925).

Article PubMed PubMed Central Google Scholar

EN ISO 1522. Paints and Varnishes: Pendulum Damping Test (ISO 1522:2006) (European Committee for Standardization, 2007).

Drelich, J. W. et al. Contact angles: History of over 200 years of open questions. Surf. Innov. 8(1–2), 3–27. https://doi.org/10.1680/jsuin.19.00007 (2020).

Article Google Scholar

Schindelin, J. et al. Fiji: An open source platform for biological image analysis. Nat. Methods 9, 676–682. https://doi.org/10.1038/nmeth.2019 (2012).

Article CAS PubMed Google Scholar

Deltombe, R., Kubiak, K. J. & Bigerelle, M. How to select the most relevant 3D roughness parameters of a surface. Scanning 36, 150–160. https://doi.org/10.1002/sca.21113 (2014).

Article CAS PubMed Google Scholar

EN 12720:2009+A1. Furniture: Assessment of Surface Resistance to Cold Liquids (European Committee for Standardization, 2014).

CEN/TS 16209. Furniture: Classification for Properties for Furniture Surfaces (European Committee for Standardization, 2022).

EN 12722. Furniture: Assessment of Surface Resistance to Dry Heat (European Committee for Standardization, 2013).

EN ISO 4624. Paints and Varnishes: Pull-Off Test for Adhesion (ISO 4624:2016) (European Committee for Standardization, 2016).

EN 152. Wood Preservatives: Determination of the Protective Effectiveness of a Preservative Treatment Against Blue Stain in Wood in Service—Laboratory Method (European Committee for Standardization, 2012).

E24-12. Standard Method for Evaluating the Resistance of Wood Product Surfaces to Mold Growth 503‒507 (American Wood Protection Association, 2014).

Johansson, P., Ekstrand-Tobin, A., Svensson, T. & Bok, G. Laboratory study to determine the critical moisture level for mould growth on building materials. Int. Biodeterior. Biodegrad. 73, 23–32. https://doi.org/10.1016/j.ibiod.2012.05.014 (2012).

Article Google Scholar

Ma, X., Qiao, Z., Huang, Z. & Jing, X. The dependence of pendulum hardness on the thickness of acrylic coating. J. Coat. Technol. Res. 10(3), 433–439. https://doi.org/10.1007/s11998-013-9477-3 (2013).

Article CAS Google Scholar

Pavlič, M., Petrič, M. & Žigon, J. Interactions of coating and wood flooring surface system properties. Coatings 11, 91. https://doi.org/10.3390/coatings11010091 (2021).

Article CAS Google Scholar

Žigon, J., Dahle, S., Petrič, M. & Pavlič, M. Enhanced abrasion resistance of coated particleboard pre-treated with atmospheric plasma. Drv. Ind. 71(2), 129–137. https://doi.org/10.5552/drvind.2020.1960 (2020).

Article Google Scholar

Phadagi, R. et al. Understanding the role of dimethylformamide as co-solvents in the dissolution of cellulose in ionic liquids: Experimental and theoretical approach. J. Mol. Liq. 328, 115392. https://doi.org/10.1016/j.molliq.2021.115392 (2021).

Article CAS Google Scholar

Levdansky, V. A., Kondrasenko, A. A., Levdansky, A. V. & Kuznetsov, B. N. Sulfation of xylan with sulfamic acid in N, N-dimethylformamide. Russ. J. Bioorg. Chem. 45, 882–887. https://doi.org/10.1134/S1068162019070057 (2019).

Article CAS Google Scholar

Kläusler, O. et al. Influence of N, N-dimethylformamide on one-component moisture-curing polyurethane wood adhesives. Int. J. Adhes. Adhes. 55, 69–76. https://doi.org/10.1016/j.ijadhadh.2014.07.019 (2014).

Article CAS Google Scholar

Cappelletto, E. et al. Wood surface protection with different alkoxysilanes: A hydrophobic barrier. Cellulose 20, 3131–3141. https://doi.org/10.1007/s10570-013-0038-9 (2013).

Article CAS Google Scholar

Juárez-Moreno, J. A., Ávila-Ortega, A., Oliva, A. I., Avilés, F. & Cauich-Rodríguez, J. V. Effect of wettability and surface roughness on the adhesion properties of collagen on PDMS films treated by capacitively coupled oxygen plasma. Appl. Surf. Sci. 349, 763–773. https://doi.org/10.1016/j.apsusc.2015.05.063 (2015).

Article CAS Google Scholar

Cogulet, A., Blanchet, P. & Landry, V. Wood degradation under UV irradiation: A lignin characterization. J. Photochem. Photobiol. B 158, 184–191. https://doi.org/10.1016/j.jphotobiol.2016.02.030 (2016).

Article CAS PubMed Google Scholar

Mokrzycki, W. S. & Tatol, M. Colour difference ΔE: A survey. Mach. Graph. Vis. 20(4), 383–411 (2011).

Google Scholar

Kubovský, I., Kačíková, D. & Kačík, F. Structural changes of oak wood main components caused by thermal modification. Polymers 12, 485. https://doi.org/10.3390/polym12020485 (2020).

Article CAS PubMed PubMed Central Google Scholar

Ganne-Chédeville, C., Jääskeläinen, A.-D., Froidevaux, J., Hughes, M. & Navi, P. Natural and artificial ageing of spruce wood as observed by FTIR-ATR and UVRR spectroscopy. Holzforschung 66, 163–170. https://doi.org/10.1515/HF.2011.148 (2012).

Article CAS Google Scholar

Gonzalez Ortiz, D. et al. Immobilization of poly(vinyl pyrrolidone) in polysulfone membranes by radically-initiated crosslinking using potassium persulfate. Membranes 12, 664. https://doi.org/10.3390/membranes12070664 (2022).

Article CAS PubMed PubMed Central Google Scholar

Mishra, K., Hashmi, S. A. & Rai, D. K. Protic ionic liquid-based gel polymer electrolyte: Structural and ion transport studies and its application in proton battery. J. Solid State Electrochem. 18, 2255–2266. https://doi.org/10.1007/s10008-014-2475-2 (2014).

Article CAS Google Scholar

Yesappa, L. et al. Optical properties and ionic conductivity studies of an 8 MeV electron beam irradiated poly(vinylidene fluoride-co-hexafluoropropylene)/LiClO4 electrolyte film for opto-electronic applications. RCS Adv. 8, 15297. https://doi.org/10.1039/c8ra00970h (2018).

Article CAS Google Scholar

Karpagavel, K. et al. Electrical properties of lithium-ion conducting poly (vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP)/Polyvinylpyrrolidone (PVP) solid polymer electrolyte. J. Electron. Mater. 50, 4415–4425. https://doi.org/10.1007/s11664-021-08967-9 (2021).

Article ADS CAS Google Scholar

Du, C.-H., Zhu, B.-K. & Xu, Y.-Y. The effects of quenching on the phase structure of vinylidene fluoride segments in PVDF-HFP copolymer and PVDF-HFP/PMMA blends. J. Mater. Sci. 41, 417–421. https://doi.org/10.1007/s10853-005-2182-6 (2006).

Article ADS CAS Google Scholar

Hao, Y. N. et al. Interface structure, precursor rheology and dielectric properties of BaTiO3/PVDF–HFP nanocomposite films prepared from colloidal perovskite nanoparticles. RSC Adv. 7, 32886. https://doi.org/10.1039/C7RA03250A (2017).

Article ADS CAS Google Scholar

Özgenç, Ö., Durmaz, S., Hakki Boyaci, I. & Eksi-Kocak, H. Determination of chemical changes in heat-treated wood using ATR-FTIR and FT Raman spectrometry. Spectrochim. Acta A Mol. Biomol. Spectrosc. 171(15), 395–400. https://doi.org/10.1016/j.saa.2016.08.026 (2017).

Article ADS CAS PubMed Google Scholar

Dyartanti, E. R., Purwanto, A., Nyoman Widiasa, I. & Susanto, H. Ionic conductivity and cycling stability improvement of PVDF/Nano-Clay using PVP as polymer electrolyte membranes for LiFePO4 batterie. Membranes 8, 36. https://doi.org/10.3390/membranes8030036 (2018).

Article CAS PubMed PubMed Central Google Scholar

You Liu, X., Timar, M. C., Varodi, A. M. & Sawyer, G. An investigation of accelerated temperature-induced ageing of four wood species: Colour and FTIR. Wood Sci. Technol. 51, 357–378. https://doi.org/10.1007/s00226-016-0867-4 (2017).

Article CAS Google Scholar

Li, X. et al. Effects of UV light irradiation on color changes in thermally modified rubber wood based on FTIR. BioResources 15(3), 5179–5197 (2020).

Article CAS Google Scholar

Rosu, D., Teaca, C.-A., Bodirlau, R. & Rosu, L. FTIR and color change of the modified wood as a result of artificial light irradiation. J. Photochem. Photobiol. B Biol. 99, 144–149. https://doi.org/10.1016/j.jphotobiol.2010.03.010 (2010).

Article CAS Google Scholar

Lei, H., Pizzi, A. & Guanben, D. Environmentally friendly mixed tannin/lignin wood resins. J. Appl. Polym. Sci. 107, 203–209. https://doi.org/10.1002/app.27011 (2008).

Article CAS Google Scholar

Kowalonek, J. & Kaczmarek, H. Studies of pectin/polyvinylpyrrolidone blends exposed to ultraviolet radiation. Eur. Polym. J. 46, 345–353. https://doi.org/10.1016/j.eurpolymj.2009.09.015 (2010).

Article CAS Google Scholar

Reinprecht, L., Tiňo, R. & Šomšák, M. The impact of fungicides, plasma, UV-additives and weathering on the adhesion strength of acrylic and alkyd coatings to the Norway spruce wood. Coatings 10, 1111. https://doi.org/10.3390/coatings10111111 (2020).

Article CAS Google Scholar

Bekhta, P., Krystofiak, T., Lis, B. & Bekhta, N. The impact of sanding and thermal compression of wood varnish type and artificial aging in indoor conditions on the varnished surface color. Forests 13, 300. https://doi.org/10.3390/f13020300 (2022).

Article Google Scholar

Gindl, M., Reiterer, A., Sinn, G. & Stanzl-Tschegg, S. E. Effects of surface ageing on wettability, surface chemistry, and adhesion of wood. Holz. Roh. Werkst. 62, 273–280. https://doi.org/10.1007/s00107-004-0471-4 (2004).

Article CAS Google Scholar

Yalcin, M. & Ceylan, M. The effects of tannins on adhesion strength and surface roughness of varnished wood after accelerated weathering. J. Coat. Technol. Res. 14(1), 185–193. https://doi.org/10.1007/s11998-016-9841-1 (2017).

Article CAS Google Scholar

Gupta, S., John, A. & Kishan Kumar, S. V. Studies on effect of coat thickness on the moisture uptake by a hardwood substrate. Maderas-Cienc. Tecnol. 18(3), 443–456. https://doi.org/10.4067/S0718-221X2016005000040 (2016).

Article CAS Google Scholar

Tu, K., Kong, L., Wang, X. & Liu, J. Semitransparent, durable superhydrophobic polydimethylsiloxane/SiO2 nanocomposite coatings on varnished wood. Holzforschung 70(11), 1039–1045. https://doi.org/10.1515/hf-2016-0024 (2016).

Article CAS Google Scholar

Pánek, M., Oberhofnerová, E., Zeidler, A. & Šedivka, P. Efficacy of hydrophobic coatings in protecting oak wood surfaces during accelerated weathering. Coatings 7, 172. https://doi.org/10.3390/coatings7100172 (2017).

Article CAS Google Scholar

Söğütlü, C., Nzokou, P., Koc, I., Tutgun, R. & Döngel, N. The effects of surface roughness on varnish adhesion strength of wood materials. J. Coat. Technol. Res. 13(5), 863–870. https://doi.org/10.1007/s11998-016-9805-5 (2016).

Article CAS Google Scholar

Vidholdová, Z. & Slabejová, G. Environmental valuation of selected transparent wood coatings from the view of fungal resistance. Ann. WULS SGGW For. Wood Technol. 103, 164–168 (2018).

Google Scholar

Download references

The authors acknowledge the financial support from the Slovenian Research Agency through research programs P4-0430 ("Forest-wood value chain and climate change: transition to circular bioeconomy"), P4-0015 ("Wood and lignocellulosic composites"), P2-0264 ("Sustainable Polymer Materials and Technologies"), P1-0099 ("Physics of soft matter, surfaces, and nanostructures"), and P4-0116 ("Microbiology and biotechnology of food and environment"). The help of Mrs. Andreja Žagar by performing the tests on blue-staining and moulds is gratefully acknowledged.

Department of Wood Science and Technology, Biotechnical Faculty, University of Ljubljana, Jamnikarjeva ulica 101, 1000, Ljubljana, Slovenia

Jure Žigon & Miha Humar

Center for Experimental Mechanics, Faculty of Mechanical Engineering, University of Ljubljana, Pot za Brdom 104, 1000, Ljubljana, Slovenia

Urška Gradišar Centa

Condensed Matter Physics Department, Jožef Stefan Institute, Jamova 39, 1000, Ljubljana, Slovenia

Maja Remškar

You can also search for this author in PubMed Google Scholar

You can also search for this author in PubMed Google Scholar

You can also search for this author in PubMed Google Scholar

You can also search for this author in PubMed Google Scholar

J.Ž.: Conceptualization, Methodology, Formal analysis, Investigation, Resources, Data curation, Writing—original draft, Writing—review and editing, Visualization. U.G.C.: Methodology, Resources, Writing—original draft, Writing—review and editing. M.R.: Methodology, Writing—review and editing, Supervision. M.H.: Methodology, Resources, Writing—review and editing, Supervision.

Correspondence to Jure Žigon.

The authors declare no competing interests.

Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Open Access This article is licensed under a Creative Commons Attribution 4.0 International License, which permits use, sharing, adaptation, distribution and reproduction in any medium or format, as long as you give appropriate credit to the original author(s) and the source, provide a link to the Creative Commons licence, and indicate if changes were made. The images or other third party material in this article are included in the article's Creative Commons licence, unless indicated otherwise in a credit line to the material. If material is not included in the article's Creative Commons licence and your intended use is not permitted by statutory regulation or exceeds the permitted use, you will need to obtain permission directly from the copyright holder. To view a copy of this licence, visit http://creativecommons.org/licenses/by/4.0/.

Reprints and Permissions

Žigon, J., Centa, U.G., Remškar, M. et al. Application and characterization of a novel PVDF-HFP/PVP polymer composite with MoO3 nanowires as a protective coating for wood. Sci Rep 13, 3429 (2023). https://doi.org/10.1038/s41598-023-30622-y

Download citation

Received: 03 January 2023

Accepted: 27 February 2023

Published: 01 March 2023

DOI: https://doi.org/10.1038/s41598-023-30622-y

Anyone you share the following link with will be able to read this content:

Sorry, a shareable link is not currently available for this article.

Provided by the Springer Nature SharedIt content-sharing initiative

By submitting a comment you agree to abide by our Terms and Community Guidelines. If you find something abusive or that does not comply with our terms or guidelines please flag it as inappropriate.

SHARE